1. Stomata
This is a small void formed by the gas that cannot escape during the metal solidification process, and its inner wall is smooth, contains gas, and has a high reflectivity to ultrasonic waves, but because it is basically spherical or ellipsoidal, that is, a point-like defect, it affects its reflection amplitude. The pores in the ingots are forged or rolled and flattened into area-type defects that are conducive to ultrasonic detection.

2.Shrinkage and looseness
When the casting or ingot is cooled and solidified, the volume is reduced, and the final solidified part is not replenished by liquid metal and a void-like defect will be formed. Large and concentrated voids are called shrinkage holes, and small and scattered voids are called loose, they are generally located in the last solidified part of the center of the ingot or casting, and their inner walls are rough, accompanied by many impurities and fine pores. Due to the law of thermal expansion and contraction, shrinkage holes are inevitable, but with different processing methods, there are different shapes, sizes and positions, and when they extend to the casting or ingot body, it becomes a defect. If the steel ingot is not cut off cleanly and brought into the forging during billet forging, it becomes a residual shrinkage hole (shrinkage hole remnant, residual shrinkage tube).
3.Slag inclusion
The slag during the melting process or the refractory material on the furnace body peels off into the liquid metal, and is rolled into the casting or ingot body during pouring, forming a slag inclusion defect. Slag inclusions usually do not exist singularly, often in dense states or dispersed at different depths, which are similar to volumetric defects but often have a certain linearity.
4.inclusion
Reaction products (such as oxides, sulfides, etc.) in the melting process - non-metallic inclusions, or the additives of some components in the metal components are not completely melted and remain to form metal inclusions, such as high-density, high-melting point components - tungsten, molybdenum, etc.
5.Segregation
Segregation in castings or ingots mainly refers to the component segregation formed during the smelting process or the melting process of metals due to uneven distribution of components, and the mechanical properties of the area where segregation exists are different from the mechanical properties of the entire metal matrix, and the difference exceeds the allowable standard range to become a defect.
6.Casting cracks
The crack in the casting is mainly caused by the shrinkage stress during the cooling and solidification of the metal exceeds the ultimate strength of the material, which is related to the shape design and casting process of the casting, and also related to the cracking sensitivity caused by the high content of some impurities in the metal material (such as hot brittleness when the sulfur content is high, cold brittleness when the phosphorus content is high, etc.). Shaft intergranular cracks will also occur in the ingot, and if they cannot be forged in the subsequent billet forging, they will remain in the forgings to become internal cracks in the forgings.
7.Cold partition
This is a unique layered defect in castings, mainly related to the casting process design of castings, it is in the pouring of liquid metal, due to splashing, churning, pouring interruption, or two strands (or strands) of metal flows from different directions meet, etc., because the semi-solid film formed by the cooling of the liquid metal surface remains in the casting body and forms a diaphragm-like area defect.
8.Peeling
This is a layered (area-type) defect formed by pouring steel ingots from ladle to ingot die during steelmaking, due to pouring interruption, pause and other reasons, the liquid metal surface poured first cools rapidly in the air to form an oxide film, and when the new poured liquid metal breaks through and turns into the ingot body when it continues to pour, it cannot be forged and eliminated.
9.anisotropy
When the casting or ingot is cooled and solidified, the cooling rate from the surface to the center is different, so different crystalline structures will be formed, which is manifested as anisotropy of mechanical properties, and also leads to anisotropy of acoustic properties, that is, there are different sound velocities and sound attenuation from the center to the surface. The presence of this anisotropy will adversely affect the size and position of the defect during ultrasonic testing of castings.